1. Core raw materials and pretreatment of filter materials
1). Fiber materials: Synthetic fibers such as polypropylene (PP) and polyester (PET) need to be dried (water content ≤ 0.1%), and natural fibers such as cotton and wool need to be degreased and disinfected.
2). Granular materials: Activated carbon, quartz sand, etc. need to be sieved and graded (particle size range 0.5-5mm), and diatomaceous earth needs to be calcined at high temperature (800℃) to increase porosity.
3). Composite substrates: For example, PTFE coated filter materials need to be plasma treated on the base fabric to enhance adhesion (peel strength ≥ 15N/cm).
The environmental humidity (RH ≤ 40%) needs to be strictly controlled during the pretreatment stage to avoid fluctuations in material properties. For example, the melt index of polypropylene fiber at 160-180℃ needs to be stable at 25-35g/10min (ASTM D1238 standard).
2. Comparison of mainstream production processes and technical parameters
1). Meltblown process
- Process: polymer melting → high-pressure airflow spinning → fiber mesh forming
- Key parameters: spinneret diameter 0.2-0.4mm, hot air temperature 230-280℃, fiber diameter 1-10μm
- Application: production of high-efficiency and low-resistance filter materials (filtration efficiency 99.9% @0.3μm, resistance ≤50Pa)
2). Needle punching process
- Process: fiber laying → multi-needle plate puncture (needle frequency 800-1200 times/min) → reinforcement into felt
- Advantages: can produce three-dimensional structure filter materials, gram weight range 100-800g/m², air permeability 5-20cm³/cm²/s
3). Sintering process
- Metal/ceramic filter materials need to be pressed into powder (pressure 20-50MPa) and then sintered at high temperature (1100-1300℃ for stainless steel and 1600℃ for alumina)
- Porosity can be controlled at 30-60%, and the temperature resistance is above 500℃

3. Post-processing technology and performance optimization
1). Surface modification:
- Hydrophobic treatment (such as fluorocarbon coating contact angle ≥120°)
- Antibacterial finishing (silver ion loading 0.5-2%)
2). Structural reinforcement:
- Ultrasonic welding (frequency 20kHz) to improve seam strength
- Hot calendering treatment to make the pore size distribution more uniform (CV value ≤15%)